Jan 8 2013
The following table shows the mechanical properties of UNS C52480 flat products as a function of heat treatment.
| Temper |
Tensile Str. |
Elong. |
| H01 |
634MPa (92ksi) |
30% |
| H02 |
758MPa (110ksi) |
20% |
| H04 |
848MPa (123ksi) |
10% |
| H06 |
896MPa (130ksi) |
6% |
| H08 |
965MPa (140ksi) |
2% |
| H10 |
1007MPa (146ksi) |
2% |
| OS015 |
517MPa (75ksi) |
55% |
The chemical composition of UNS C52480 copper alloy is outlined in the following table.
| Element |
Content (%) |
| Tin, Sn |
10 - 11 |
| Zinc, Zn |
0.3 |
| Iron, Fe |
0.05-0.2 |
| Nickel, Ni |
0.05–0.2 |
| Lead, Pb |
0.05 |
| Phosphorous, P |
0.01-0.35 |
| Copper, Cu |
Remainder |
Copper and the elements mentioned in the above table together constitute 99.5% of this alloy.