Jan 3 2013
Copper UNS C84200 has a copper content of not less than 82%.
The following table shows the mechanical properties of UNS C84200 sand cast alloy as a function of heat treatment.
Temper |
Tensile Str. |
Yield Str. |
Elong. |
M01 |
241MPa (35ksi) |
97MPa (14ksi) |
27% |
Equivalent materials to the UNS C84200 copper alloy are the following:
- ASTM B30
- ASTM B505
- QQ C390
The chemical composition of UNS C84200 copper alloy is outlined in the following table.
Element |
Content (%) |
Copper, Cu |
78-82 |
Zinc, Zn |
10-16 |
Tin, Sn |
5-6 |
Lead, Pb |
2-3 |
Nickel, Ni |
0.8 |
Iron, Fe |
0.4 |
Antimony, Sb |
0.25 |
Sulfur, S |
0.08 |
Phosphorous, P |
0.05 |
Silicon, Si |
0.005 |
Aluminum, Al |
0.005 |