Dec 20 2012
UNS C84800 has a copper content of not less than 75%.
Tabulated below are the mechanical properties of UNS C84800 copper sand cast alloy as a function of heat treatment.
| Temper |
Tensile Str. |
Yield Str. |
Elong. |
Rockwell |
Fatigue Str. |
| B |
C |
F |
30T |
| M01 |
255MPa (37ksi) |
97MPa (14ksi) |
35% |
- |
- |
- |
- |
76MPa (11ksi) |
| M07 |
193MPa (28ksi) |
83MPa (12ksi) |
16% |
- |
- |
- |
- |
- |
The chemical composition of UNS C84800 copper alloy is outlined in the following table.
| Elements |
Content (%) |
| Copper, Cu |
75.0-77.0 |
| Zinc, Zn |
13.0-17.0 |
| Lead, Pb |
5.5-7.0 |
| Tin, Sn |
2.0-3.0 |
| Nickel, Ni |
1.0 |
| Iron, Fe |
0.4 |
| Antimony, Sb |
0.25 |
| Sulfur, S |
0.08 |
| Phosphorus, P |
0.02 |
| Silicon, Si |
0.005 |
| Aluminum, Al |
0.005 |
Equivalent materials to UNS C84800 copper alloy are:
- ASTM B271
- ASTM B30
- ASTM B505
- ASTM B584
- ASTM B763
- QQ C390