Sep 27 2012
The following table shows the mechanical properties of UNS C50715 flat products as a function of heat treatment.
| Temper |
Tensile Str. |
Elong. |
| H02 |
393MPa (57ksi) |
15% |
|
503MPa (73ksi) |
25% |
| H04 |
510MPa (74ksi) |
8% |
|
600MPa (87ksi) |
16% |
| H06 |
558MPa (81ksi) |
5% |
|
655MPa (95ksi) |
10% |
| H08 |
593MPa (86ksi) |
3% |
|
689MPa (100ksi) |
6% |
| H10 |
517MPa (75ksi) |
- |
|
579MPa (84ksi) |
- |
The chemical composition of UNS C50715 copper alloy is outlined in the following table.
| Element |
Content (%) |
| Tin, Sn |
1.7-2.3 |
| Iron, Fe |
0.05-0.15 |
| Phosphorous, P |
0.025-0.04 |
| Lead, Pb |
0.02 |
| Copper, Cu |
Balance |
Copper, tin, iron and lead together constitute a minimum of 99.5% of this alloy.