The key properties of polyaramid fibre reinforced polyphenylene sulphide composite are tabulated below.

Table 1. Key properties

Mechanical Properties

Elongation at break ( % )

1.5

Thermal expansion coefficient - long. ( x10-6 strain K-1 )

27

Young's modulus - transverse ( GPa )

9.6

Properties Polyaramid/Polyphenylenesulphide Composite Sheet

Property

Value

Compressive Strength - Longitudinal

MPa

76

Density

g cm-3

1.25

Flexural modulus - Longitudinal

GPa

7.6

Flexural strength - Longitudinal

MPa

124

Tensile strength - Longitudinal

MPa

83

Volume fraction of fibres

%

~25

Properties Polyaramid/Polyphenylenesulphide Composite Rod

Property

Value

Compressive Strength - Longitudinal

MPa

76

Density

g.cm-3

1.25

Flexural modulus - Longitudinal

GPa

7.6

Flexural strength - Longitudinal

MPa

124

Tensile strength - Longitudinal

MPa

83

Volume fraction of fibres

%

25

About Goodfellow

Goodfellow supplies metals, ceramics and other materials to meet the research, development and specialist production requirements of science and industry worldwide.

Source: Goodfellow.

For more information on this source please visit Goodfellow.

Tell Us What You Think

Do you have a review, update or anything you would like to add to this article?

Leave your feedback
Your comment type
Submit